C | Si | Mn | Cr | Mo | W | V | Al | P | S |
0.65~0.75 | ≤0.80 | 14.5~16.0 | 2.0~2.5 | 0.5~0.8 | 0.5~0.8 | 1.5~2.0 | 2.7~3.3 | ≤0.04 | ≤0.03 |
溫度/℃ | 25~100 | 25~200 | 25~300 | 25~400 | 25~500 | 25~600 | 25~700 | 25~800 | 25~900 |
線(膨)脹系數(shù)/℃-1 | 16.0 | 17.8 | 18.9 | 19.7 | 20.3 | 20.8 | 21.2 | 21.6 | 21.6 |
溫度/℃ | 150 | 300 | 400 | 500 | 600 | 700 | 800 | 900 |
熱導(dǎo)率λ/w·(m·k)-1 | 14.4 | 15.7 | 19.5 | 20.0 | 20.3 | 22.2 | 24.9 | 24.8 |
溫度/℃ | 150 | 300 | 400 | 500 | 600 | 700 | 800 | 900 |
電阻率/Ω·m | 1.05×10-6 | 1.15×10-6 | 1.17×10-6 | 1.23×10-6 | 1.25×10-6 | 1.31×10-6 | 1.33×10-6 | 1.35×10-6 |
狀 態(tài) | 磁導(dǎo)率μ/mH·m-1 |
1150℃固溶 1180℃固溶 1150℃固溶,700℃2h時(shí)效 1180℃固溶,650℃20h時(shí)效 1180℃固溶,700℃2h時(shí)效 1180℃固溶,650℃20h時(shí)效,變形8.5% 1180℃固溶,650℃20h時(shí)效,變形14.5% 1180℃固溶,650℃20h時(shí)效,變形24.2% 1180℃固溶,650℃20h時(shí)效,變形42.2% |
1.2602×10-3 1.2603×10-3 1.2639×10-3 1.2607×10-3 1.2602×10-3 1.2608×10-3 1.2608×10-3 1.2617×10-3 1.2704×10-3 |
項(xiàng)目 | 加熱溫度/℃ | 加熱時(shí)間/℃ | 開鍛時(shí)間/℃ | 終鍛溫度/℃ | 冷卻方式 |
鋼錠 鋼坯 |
1150~1170 1140~1160 |
≥8 ≥8 |
1100~1120 1090~1110 |
≥950 ≥950 |
空冷 空冷 |
熱處理制度 | σb/MPa | δ/% | ψ/% | αK/J·cm-1 |
1180℃固溶 |
820 720 |
61.0 60.0 |
61.5 62.5 |
230 240 240 |
1150℃固溶,700℃2h時(shí)效 |
1370 1370 1380 |
16.5 15.5 18.0 |
34.0 35.5 35.5 |
48 45 45 |
1165℃固溶,700℃2h時(shí)效 |
36 39 40 |
|||
1180℃固溶,700℃2h時(shí)效 |
1510 1490 |
4.5 4.5 |
8.5 9.5 |
15 13 13 |
固溶溫度/℃ | 保溫時(shí)間/℃ | 冷卻介質(zhì) | 固溶硬度(HRC) |
1150~1160 | 鹽溶爐1520或空氣爐 | 水 | 20~22 |
狀態(tài) | 鍛造 | 退火 | 固溶 | 時(shí)效 |
硬度(HRC) | 33~35 | 28~30 | 20~22 | 47~48 |
時(shí)效溫度/℃ | 保溫時(shí)間/h | 冷卻介質(zhì) | 時(shí)效硬度(HRC) |
650 700 |
20 2 |
空氣 空氣 |
48.0 48.5 |
氮化溫度/℃ | 氮化時(shí)間/℃ | 氮化層深度/mm | 氮化層硬度(HRC) |
560~570 | 4~6 | 0.03~0.03 | 950~1100 |